BS X2CrNiMoN17-13-5
2015-04-08 08:50:58 Origin: Remark:0 Click:
BSEN Austenitic stainless steel material specification X2CrNiMoN17-13-5 datasheet,X2CrNiMoN17-13-5 Chemical, Ring forging,X2CrNiMoN17-13-5 Bar, Wire rod, Sheet - steelmaking,BS X2CrNiMoN17-13-5 ESR, Blooming, Forging, Rolling, Heat treatment, Straightened, Ultrasonic test, Cold working, Machined. We also possess advanced precision machining equipments for further processing.
Technical Standards - BS EN 10088-3 (2005) or by agreement.
OFFICIAL TEST CERTIFICATE: issued by TUV - SGS - BV
TECHNICAL SPECIFICATION / DATASHEET - BS X2CrNiMoN17-13-5 /1.4439
MATERIAL CATEGORY: Stainless steel round bar, wire rod, and semi-finished products
STEEL TYPE: Austenitic series
MATERIAL SPECIFICATIONS: BS EN 10083-3 (2005)
CHEMICAL COMPOSITION (WEIGHT %)
C(%): ≤0.030
Si(%): ≤1.00
Mn(%): ≤2.00
P(%)≤: 0.045
S(%)≤: 0.015
Cr(%): 16.5~18.5
Ni(%): 12.5~14.5
Mo(%): 4.00~5.00
Si(%): ≤1.00
Mn(%): ≤2.00
P(%)≤: 0.045
S(%)≤: 0.015
Cr(%): 16.5~18.5
Ni(%): 12.5~14.5
Mo(%): 4.00~5.00
Other(%): N 0.12~0.22
MECHANICAL PROPERTIES ( BAR/WIRE ROD ) AND INTERGRANULAR CORROSION RESISTANT TENDENCY VIA SOLUTION TREATMENT
Thickness Diameter (d)/≤mm: 160
Hardness HBS: 250
Yield strength σ0.2≥/MPa: 280
Tensile strength σb/MPa: 580~700
Yield strength σ0.2≥/MPa: 280
Tensile strength σb/MPa: 580~700
Elongation δ(longitudinal )≥(%): 35
Elongation δ(transversal )≥(%): -
Impact absorbing energy Akv≥/J|longitudinal: 100
Impact absorbing energy Akv≥/J|transversal: -
Intergranular corrosion resistance tendency | condition of delivery: Yes
Intergranular corrosion resistance tendency | condition of welding: Yes
Impact absorbing energy Akv≥/J|transversal: -
Intergranular corrosion resistance tendency | condition of delivery: Yes
Intergranular corrosion resistance tendency | condition of welding: Yes
Thickness Diameter (d)/≤mm: 160<d≤250